Straight answers to the questions people ask most when choosing and using 5183 aluminium MIG wire.
What is 5183 aluminium MIG wire and what is it used for?

5183 is an aluminium-magnesium filler wire with roughly 4.5 to 5 per cent magnesium and a little manganese, classified as ER5183. The manganese gives a higher-strength weld metal than the common 5356 wire. It is mainly used for welding the high-magnesium 5000 series plate alloys, such as those used in shipbuilding, marine work, tanks and transport structures.
It is not a general-purpose wire for every aluminium job. For other alloys, check the filler recommended for the parent metal before you choose it.
How is 5183 different from 5356 wire?

Both are aluminium-magnesium wires and both are very widely used. 5183 contains manganese and is generally chosen when the highest as-welded strength is needed on high-magnesium plate such as 5083, and where the job or a classification society specifies it. 5356 is the more general-purpose wire, and is commonly used on 5000 and 6000 series material.
If the welding procedure or drawing names a filler, use that one. If not, check the filler selection charts from the wire maker or a standards body for your parent alloy.
Which base alloys is 5183 normally used on?

It is mostly used on the higher-magnesium 5000 series alloys such as 5083, 5086 and 5456, and sometimes on lower-magnesium 5000 series material such as 5052. It is not normally chosen for 1000, 3000 or 6000 series alloys, where other fillers give better results.
Parent alloy, temper, thickness and service conditions all influence the filler choice, so check a filler selection chart and your welding procedure rather than relying on the alloy number alone.
Can I use 5183 for parts that run hot?

Generally no. Aluminium-magnesium fillers with more than about 3 per cent magnesium, including 5183, can become prone to stress corrosion cracking if the weld sees service temperatures above about 65 degrees C for long periods, especially in a corrosive environment such as salt water.
For parts that stay warm in service, a lower-magnesium filler is the usual alternative, although it gives lower strength. Check the maker's data sheet and the governing specification for your application.
Why does aluminium wire feed badly, and how do I fix it?

Aluminium wire is soft, so it is easily crushed, scraped or tangled in the cable, which causes erratic feeding and the wire bunching at the drive rolls (often called bird-nesting). Use U-groove or soft V-groove drive rolls, lower the roll pressure than you would use for steel, and fit a plastic liner such as nylon or PTFE instead of a steel one, which can scratch the wire and shed fine shavings.
Keep the cable short and straight, make sure the contact tip suits aluminium, and keep the liner clean. A guide tube between the rolls and the liner also helps.
Do I need a push-pull gun or spool gun?

Not always. A standard push feed system can handle aluminium, particularly with larger wire diameters and a short torch cable. Thin, soft wire is harder to push, and long cable runs make it worse.
A push-pull torch, with a motor in the handle to help pull the wire, or a spool gun that carries a small spool of wire on the torch, makes feeding more reliable on thinner wire and longer reaches. 5183 is a little stiffer than the softest aluminium wires, but the same advice applies. Check what your machine supports.