Straight answers to the questions people ask most when TIG welding mild and medium tensile steel with ER70S-2 wire.
Why is ER70S-2 popular for pipe root passes?

ER70S-2 is a copper-coated steel rod that is deoxidised with several elements (triple deoxidised): zirconium, titanium and aluminium are added on top of the usual silicon and manganese. The extra deoxidisers help the weld pool cope with the small amounts of oxygen and surface contamination that are hard to avoid at a root, which helps give a clean, sound weld bead with less porosity.
That is why makers list root-pass pipe welding, small-bore pipe and tube among its typical uses on mild and low alloy steel. Your welding procedure may name the filler for the root and for the following passes, so check it first.
What strength weld metal does ER70S-2 give and which steels does it suit?

The 70 in the name refers to a minimum tensile strength of 70 thousand pounds per square inch, about 480 MPa. Maker data sheets also list a minimum yield strength of about 400 MPa and a minimum elongation of 22%, tested as the classification requires. Typical as-welded results are usually higher than these minimums.
It is a good match for mild steel and the medium tensile structural and pipe steels, rather than for high-strength or alloyed steels. For higher strength steels or special requirements, check the job specification, and where certificates are required the batch certificate shows the properties you can rely on.
What current, polarity and tungsten should I use with ER70S-2?

ER70S-2 is welded with direct current, electrode negative (DC-), using a pure argon shield. For steel, ceriated or lanthanated tungsten is a good choice, ground to a point with the grind marks running lengthwise along the electrode.
Thoriated tungsten is slightly radioactive. The main concern is inhaling grinding dust, so use a dedicated grinder with local dust extraction, or choose ceriated or lanthanated types, which are accepted alternatives. Set the current for the thickness and joint, and follow the maker's and your procedure's guidance.
What causes porosity when TIG welding steel, and how do I avoid it?

In TIG welding, porosity is most often caused by a loss of gas shield or by contamination. Typical culprits are a leak in the gas line or a loose fitting, too high a gas flow that causes turbulence, draughts in the work area, and grease, oil, paint, rust or moisture on the joint or the rod.
Check the hoses and connections, set the flow as the maker advises rather than as high as possible, screen the work from draughts, keep the torch close enough to hold the shield, and clean the joint and the rod before you weld.
Does ER70S-2 give good toughness for low-temperature service?

The classification includes an impact (toughness) requirement: maker data sheets quote a minimum of 27 J at about minus 30 degrees C, with typical as-welded results well above that. So it is often used where reasonable toughness matters.
The classification test is done with a stated shielding gas, and actual results depend on the gas, the heat input, the number of passes and the base steel. If your job has a minimum impact value at a stated temperature, check the batch certificate and the qualified welding procedure, and do not assume the rod will meet it in every set-up.
Can I use ER70S-2 to join steel to stainless steel?

It is not what is recommended. ER70S-2 is a plain carbon steel filler. Guidance on joining stainless steel to carbon or low alloy steel is to use an austenitic filler that matches the stainless grade, or a nickel-based filler. Dilution from the carbon steel can otherwise produce hard, brittle structures in the weld, which is why an over-alloyed stainless filler is often used for these joints.
The right filler depends on the stainless grade, the steel and the service conditions, so use the filler named in your procedure or ask for advice before you weld.
Why can thick-walled pipe crack hours after it has been welded?

This is usually hydrogen cracking. It needs three things together: hydrogen from the welding process, a hard brittle structure in the steel, and tensile stress. The crack can appear after the weld has cooled to ambient temperature, sometimes some hours later.
Thick sections and steels with a higher carbon content or higher alloy content are more at risk. Preheat, controlled interpass temperature, clean and dry materials and sometimes a post-weld hold can all reduce the risk, and the right levels depend on the steel and the thickness. Follow your welding procedure and the applicable code.