Hard Facing MIG Wire FAQs
Straight answers to the questions buyers ask most when choosing and using hardfacing cored wire for wear-resistant overlays.
What is the difference between chromium carbide, martensitic and manganese hardfacing wires?

Chromium carbide deposits are the usual choice for abrasion with low to moderate impact. They are very hard but brittle, so they tend to show fine cracks and are usually limited in how many layers can be built up.
Martensitic deposits are a compromise: good abrasion resistance with better toughness, so they suit mixed abrasion and impact, and they are often used as a build-up as well. Austenitic manganese deposits are tough and harden under hammering, so they suit heavy impact and rebuilding manganese steel parts, but they are not the best choice for pure sliding abrasion. Always check the maker's data sheet for the alloy you are considering.
Do I need a buffer layer before hardfacing?

Often, yes. A buffer or build-up layer gives the hard deposit a tough, crack-resistant base, and it is commonly used on steels that harden easily and when rebuilding worn parts. The buffer must be compatible with both the base metal and the final hardfacing alloy.
On manganese steel, an austenitic buffer is normally used rather than a carbon steel build-up. Before welding, remove the old work-hardened surface from manganese steel, because leaving it in place can cause cracking under the weld. If a wire's data sheet specifies a buffer layer for your base metal, follow it.
Do I need to preheat before hardfacing?

It depends on the base metal. Higher-carbon and low-alloy steels, tool steels, martensitic stainless steels and most cast irons are normally preheated, and the amount depends on the carbon and alloy content, the thickness and the wire. Preheating also helps reduce distortion and cracking, and slow cooling afterwards helps protect the heat-affected zone.
Austenitic manganese steel is different. It should not be preheated much and should not be allowed to get too hot, because excessive heat makes it brittle, so keep the base metal below the maximum temperature the maker gives. Always follow the wire maker's data sheet and your welding procedure.
Is it normal for a hardfacing deposit to crack?

With chromium carbide types, fine cracks running across the beads (check cracking) are usually normal. They form as the hard, brittle deposit cools and contracts, and they relieve stress. They are generally not harmful to wear performance unless the part sees a corrosive service.
Cracks that run along the bead, or that go down into the base metal (underbead cracking), are a warning sign. They can lead to the deposit breaking away. Common causes are too little dilution with the base metal, no buffer layer, too little preheat or cooling too quickly. If your deposit shows irregular cracking, review the procedure and the data sheet.